Manuscript Offprint
arXiv:2611.04707Methodological Assessment of Instrumented Indentation for Spatially Resolved Mesoscale Stiffness and Creep in Short Fiber-Reinforced Injection-Molded PBT Components
ABSTRACT
Instrumented indentation enables assessment of local mechanical properties in heterogeneous polymer systems, but specimen preparation and the selected indentation protocol significantly influence the quantitative interpretation of the measured response. This study develops and evaluates an experimental methodology for spatially resolved mesoscale characterization of both unreinforced and short fiber-reinforced composites. An unreinforced material system is used as a reference material to systematically examine the effects of indentation spacing, surface preparation, maximum indentation load, temporal loading parameters, and unloading evaluation. Indentation loads of 500 mN, 1000 mN, and 1750 mN are investigated in complementary experimental campaigns. The apparent indentation modulus exhibits moderate sensitivity to indentation load and loading time within the studied ranges. In contrast, indentation depth and the creep-related depth increment display greater sensitivity to the applied load history. Surface polishing minimizes topographical disturbances and enables reliable identification of residual indentation profiles and pile-up. Based on these methodological findings, a final load-hold-unload protocol with an indentation load of 1750 mN, a loading time of 6 s, a holding period of 300 s, and an unloading time of 4 s is applied to both unreinforced material and short fiber-reinforced composites. The mean apparent indentation modulus increases from 2.91 GPa for unreinforced material to 6.65 GPa for short fiber-reinforced composites, while the mean depth of indentation creep decreases from 2.36 µm to 1.91 µm. The coefficient of variation also increases for both quantities, indicating that short-fiber reinforcement enhances mean local stiffness and introduces pronounced spatial heterogeneity in both stiffness-related and time-dependent mesoscale indentation responses.
1 | Introduction
Short-fiber-reinforced composites (SFRCs) are widely used in mechanically loaded components because they combine low density, efficient processability, and relatively high stiffness and strength. Injection-molded SFRCs, in particular, present considerable potential for lightweight structural applications with complex geometries. This study examines two injection-molded polybutylene terephthalate (PBT) material systems: unreinforced PBT (PBT GF0) and short-glass-fiber-reinforced PBT with a nominal glass-fiber mass fraction of 30 wt.% (PBT GF30). Both systems utilize the same thermoplastic matrix, which allows for a direct
comparison of the effects of short-glass-fiber reinforcement on the local mechanical response at the mesoscale.
The mechanical behavior of PBT GF30 is influenced not only by the properties of the polymer matrix and reinforcement but also by the heterogeneous microstructure formed during injection molding. Variations in fiber content, fiber orientation, matrix morphology, and fiber-matrix interactions produce spatially heterogeneous mechanical properties. This heterogeneity is especially pronounced in the characteristic skin-core morphology of injection-molded SFRCs, where flow-induced shear aligns fibers predominantly along the melt-flow direction in the outer layers, while more transverse or less strongly aligned fiber orientations are observed in the core [1, 2].
Copyright Statement © 2024 XXXX
Submitted for Publication, 2026;v0:1-22 https://doi.org/0000
1 of 22
This heterogeneity becomes particularly important when the polymer matrix exhibits time-dependent behavior. Thermoplastic matrices undergo viscoelastic deformation under sustained mechanical loading, while the incorporation of stiff fibers modifies both the overall stiffness and the resulting time-dependent deformation. Consequently, characterization based only on spatially averaged component-level properties does not adequately capture the local material response required for micromechanical analysis or spatially resolved material modeling [31].
Instrumented indentation is an effective technique for investigating mechanical behavior at the mesoscale. During these experiments, the continuously recorded force-displacement response allows for the determination of local stiffness-related properties from the unloading segment and facilitates the assessment of time-dependent deformation by analyzing displacement evolution under sustained load. The Oliver-Pharr methodology is commonly employed to evaluate indentation modulus and hardness from indentation measurements [42, 43]. Furthermore, extended holding segments at maximum load enable quantification of the time-dependent response of SFRC through indentation creep measurements [60].
The indentation response of polymers is highly sensitive to experimental and evaluation parameters [17], e.g. the quantitative indentation response of polymers is sensitive to specimen surface condition, maximum load, and testing speed [25]. Surface roughness affects initial contact detection and local contact geometry. Insufficient spacing between adjacent indentations can lead to interactions with previously plastically deformed regions. Additionally, the loading rate, holding period, unloading duration, and the chosen unloading-curve range influence the evaluated indentation modulus, as time-dependent deformation may persist throughout the entire indentation cycle [17, 21]. Hence, the prescribed load-hold-unload history and the unloading rate can significantly influence the separation of elastic and time-dependent deformation [29, 52, 53]. Direct observations of viscoelastoplastic polymers also indicate that sink-in and pile-up phenomena can coexist during the indentation cycle, resulting in contact geometries that may deviate from the assumptions of conventional Oliver-Pharr evaluation [39, 54, 60].
Spatial indentation is a well-established method for characterizing heterogeneous polymers and polymer-matrix composites [12, 14]. For instance, Rauter [48] demonstrated spatially resolved indentation modulus mapping of injection-molded SFRC on the mesoscale and quantified the effective material region represented by the indentation response. Furthermore, indentation creep has been applied to SFRC [55] and has also been reported for polymers filled with glass fiber in studies of radiation-induced material modification [45].
These methodological factors are particularly critical when interpreting spatial variations in indentation properties as indicators of intrinsic material heterogeneity [33, 49]. It is essential to distinguish experimental scatter resulting from surface preparation or inappropriate indentation parameters from the true spatial variability of the material under investigation [17]. Therefore, a consistent indentation protocol should be established prior to statistical evaluation of differences between unreinforced material and SFRC.
The current literature lacks an integrated experimental methodology that systematically assesses the influence of surface preparation, indentation spacing, maximum load, temporal test parameters, and unloading evaluation, followed by the application of a unified protocol to spatially map both the apparent indentation modulus and the long-hold indentation creep response of matched unreinforced material and SFRC. This study addresses this gap by combining a systematic methodological assessment with a spatially resolved application to injection-molded PBT. Unreinforced PBT GF0 is used as the reference system to evaluate indentation spacing, surface preparation, indentation load, temporal test parameters, and unloading evaluation. Based on these measurements, a final indentation protocol is developed and applied to both PBT GF0 and glass fiber reinforced PBT GF30. Subsequent analyses focus on the apparent indentation modulus and the absolute indentation creep depth increment . Here, spatially distributed measurements on polished specimen cross-sections are conducted to determine mean values, standard deviations, coefficients of variation (CoV), and spatial distributions of and . This approach enables a quantitative assessment of the influence of short-fiber reinforcement on both the average local response and its spatial variability. Additionally, the spatially resolved measurements yield statistical descriptors and spatial response maps of local material behavior, providing an experimental foundation for subsequent stochastic analyses that explicitly consider spatial material variability [44].
Accordingly, the remainder of this paper is organized as follows. Section 2 provides the main theoretical aspects. All information about the investigated material systems, specimen preparation, and the used laboratory testing equipment are introduced in Section 3. Section 4 presents and discusses the methodological assessment performed on PBT GF0 and consolidates their implications into the final indentation protocol. The spatially resolved results for PBT GF0 and PBT GF30 are presented in Section 5 including the discussion of the material-related findings and its limitations. This is followed by the main conclusions in Section 6.
2.1 | Scale separation and mesoscale indentation concept
Following the multi-scale concept, the mechanical response of SFRC is influenced by the spatial scale at which the heterogeneous microstructure is examined. At the microscale, individual constituents and their interfaces are explicitly resolved. In contrast, structural testing at the component level yields an effective response averaged over a larger representative material volume. Between these two extremes, a mesoscale description characterizes the apparent local response of a heterogeneous material region without resolving each constituent individually [6, 44, 50, 62].
For a heterogeneous material with characteristic microstructural length l, mesoscale length d, and characteristic component dimension L, the classical separation-of-scales condition is expressed as [24, 65]
2 of 22

FIGURE 1 | A schematic illustration demonstrates scale separation in a short-fiber-reinforced composite. The macroscopic component is defined by the length scale , while the local material region , bounded by and characterized by dimension , contains glass fibers embedded within the polymer matrix. The characteristic microstructural length represents the scale of the underlying heterogeneities. The elastic moduli of the fibers and matrix are denoted as and , respectively. The coordinate systems and correspond to the component level and local material descriptions, respectively.
Figure 1 schematically illustrates the corresponding scale hierarchy and the relationship between the macroscopic component and the local heterogeneous material region.
In this context, denotes the characteristic length of the microstructural heterogeneity, including the glass fibers and their spatial arrangement, whereas represents the macroscopic specimen or component-level dimension. Under the assumed separation of scales, the intermediate length characterizes the mesoscale, at which the apparent local mechanical response reflects the collective influence of the heterogeneous microstructure rather than the properties of individual constituents [50].
The characteristic microstructural length scale differs fundamentally between the two material systems examined in this study. In unreinforced PBT (PBT GF0), is determined by the polymer matrix morphology, including semi-crystalline domain and spherulite sizes as well as the arrangement of crystalline lamellae, and typically falls within the sub-micron to low-micrometer range [14, 29]. For a given projected indentation area, the resulting scale ratio is therefore very large, so the indentation process samples an effectively homogeneous material continuum. In contrast, in PBT GF30, the characteristic length is defined by the mean diameter of the glass fibers () and their spatial distribution. Under identical indentation loads and projected contact areas, the indentation-affected volume in PBT GF30 contains only a few fibers and adjacent matrix regions. Thus, the ratio is much smaller for PBT GF30, rendering the mesoscale response highly sensitive to local microstructural variations and contributing to the observed experimental parameter scatter.

FIGURE 2 | Schematic force-displacement response during instrumented indentation illustrates the loading, holding, and unloading segments. During the holding period at , the indentation depth increases from to , which defines the indentation creep depth increment . The contact stiffness is determined from the initial unloading slope. The parameter indicates the extrapolated residual depth, while refers to the calculated contact depth as described in [42, 43].
Instrumented indentation is applied within the mesoscale regime in this study. The volume of material affected by each indentation comprises contributions from the polymer matrix and, for PBT GF30, from locally varying fiber configurations that constrain the expanding elastic-plastic deformation fields [12, 57]. Consequently, the measured response is interpreted not as a phase-specific constituent property but as an apparent local response associated with the indentation-affected material region [6, 50]. Spatial repetition of this measurement across the specimen cross-section provides a mesoscale representation of local mechanical variability while preserving positional context within the macroscopic specimen.
2.2 | Indentation modulus and indentation creep
Instrumented indentation measurements were evaluated using the recorded indentation force and indentation depth . All experiments employed a Berkovich diamond indenter. The apparent indentation modulus was determined from the unloading phase of the force-displacement response using the Oliver-Pharr approach [42, 43].
Figure 2 schematically illustrates the characteristic force-displacement response during a load-hold-unload indentation cycle. The holding segment at constant maximum load quantifies the additional time-dependent indentation displacement, while the subsequent unloading response provides the contact stiffness needed to determine the apparent indentation modulus .
The unloading curve is approximated using a power-law relation of the form
where and are fitting parameters, and denotes the residual indentation depth obtained by extrapolating the unloading curve. The contact stiffness is subsequently evaluated from the
3 of 22 derivative of Equation (2) at the maximum indentation depth,
Based on Sneddon's analytical solution for the boundary deflection of an elastic half-space [59], the corresponding contact depth is calculated as
Here, denotes the maximum indentation load, and is the contact-depth correction coefficient adopted for the Berkovich indentation evaluation [26, 42, 60]. Figure 3 schematically illustrates the influence of sink-in and pile-up on the contact geometry. The conventional Oliver-Pharr contact-depth approximation accounts for sink-in; however, pile-up can result in the actual contact depth and projected contact area exceeding their estimated values.

FIGURE 3 | Schematic comparison of pile-up and sink-in during instrumented indentation. Pile-up produces upward displacement of material around the indenter, potentially increasing the actual geometrical contact depth and projected contact area beyond the values estimated using the conventional Oliver-Pharr procedure. In contrast, sink-in produces a downward displacement of the surrounding surface, which is accounted for by the conventional contact-depth approximation under the assumed elastic contact conditions [42, 43].
The projected contact area is determined using the calibrated area function of the Berkovich indenter, which accounts for deviations from the ideal pyramidal geometry, including the finite tip radius [43]. Because the estimated contact depth may be inaccurate in the presence of pile-up, the resulting indentation modulus is interpreted as an apparent material property at the mesoscale. The associated limitations are discussed in Section 2.3.
Assuming an isotropic contact relation, the reduced indentation modulus is given by
In this context, a symmetry correction factor of is incorporated. This assumption is widely accepted for Berkovich geometries [19, 50, 61].
The indentation modulus of the specimen is calculated by accounting for the elastic properties of the diamond indenter and the reduced indentation modulus, as expressed by
Here, GPa and denote the Young's modulus and Poisson's ratio of the indenter [42], respectively, while refers to the assumed Poisson's ratio of the specimen. For PBT GF0, the Poisson's ratio is [49], and for PBT GF30, [48].
In addition to the stiffness-related response, the time-dependent indentation behavior is evaluated using the holding segment at to address the pronounced viscoelasticity of the polymer matrix [17, 58, 60]. The indentation depth at the beginning of the holding period is denoted as , while represents the maximum indentation depth reached at the end of the holding period. The increment in absolute indentation creep depth is defined as
This value quantifies the additional indentation depth accumulated during the holding period and is used as the primary measure of the time-dependent indentation response in this study. To account for the indentation depth already reached at the beginning of the holding period, the relative indentation creep is additionally defined as [58]
Here, denotes the indentation depth at the beginning of the holding period. The relative indentation creep describes the percentage increase in indentation depth during the constant-load holding period. In contrast to , which is expressed in units of length, provides a dimensionless measure of the time-dependent indentation response.
2.3 | Evaluation limitations associated with pile-up and viscoelastic unloading
The Oliver-Pharr evaluation method assumes that the projected contact area is determined from the contact depth and the elastic unloading response. Although this approach accounts for elastic sink-in around the indenter, it becomes inaccurate when material is displaced upward around the residual indentation imprint, resulting in pile-up [18, 42, 43, 60]. In these cases, the actual projected contact area can exceed the area estimated from , leading to an underestimation of the contact area and a corresponding overestimation of the derived modulus and hardness [3, 39, 47]. This limitation is particularly relevant for polymers and polymer-matrix composites, where plastic and time-dependent deformation may persist throughout the indentation cycle [17, 60]. In SFRC, the heterogeneous fiber-matrix microstructure may additionally modify the local deformation field and the resulting surface displacement around the indenter [17, 18]. Within this work, the residual surface geometry was not used to correct the projected contact area, and no pointwise contact-area correction was performed for the spatial indentation measurements. Consequently, the resulting modulus is consistently interpreted as an apparent indentation modulus .
A second limitation arises from ongoing time-dependent deformation during unloading. If the viscoelastic displacement rate remains significant at the transition from the holding segment to unloading, the initial curvature of the force-displacement response may deviate from the predominantly elastic unloading response assumed in conventional evaluation. In severe cases,
4 of 22 this persistent creep deformation can result in a negative initial unloading slope, commonly referred to as the viscoelastic "nose" effect, which precludes standardized stiffness determination [29, 60]. Consequently, the choice of the fitting interval in the unloading phase can substantially affect the calculated contact stiffness S and, therefore, .
2.4 | Statistical measures
Spatial indentation data were analyzed using descriptive statistical measures to differentiate changes in mean local response from variations in spatial variability. For a quantity X measured at n valid indentation positions, the arithmetic mean is defined by
The sample standard deviation is calculated as
and the CoV is obtained from
The CoV facilitates a scale-independent comparison of relative spatial scatter between PBT GF0 and PBT GF30, as the mean values of both and differ substantially between these material systems due to the stiffening effect of the short-fiber reinforcement [10].
3 | Experimental setup
3.1 | Material systems and specimen definition
The material system investigated in this study consists of a PBT matrix based on Ultradur B 4520 and short E-glass fibers as the reinforcement phase. This material system was used to produce two sets of injection-molded standardized tensile specimens conforming to DIN EN ISO 527-2 type 1A at Kunststoff-Zentrum Leipzig gGmbH using an Arburg Allrounder 370E injection molding machine. The injection-molding parameters are detailed in [34]. Both PBT GF0, designating the unreinforced specimens, and PBT GF30, a reinforced material system with a nominal short-fiber mass fraction of 30 wt.%, specimens were manufactured with identical nominal geometries, as depicted in Figure 4, and comparable processing conditions to provide a consistent experimental basis for the subsequent indentation investigations.
PBT GF0 serves as a comparatively homogeneous reference system for evaluating methodological influences, as it does not exhibit the local variability introduced by glass fibers at the mesoscale. In contrast, the indentation response of PBT GF30 reflects the apparent local behavior of a heterogeneous material volume, incorporating varying contributions from the polymer matrix, glass fibers, and adjacent fiber-matrix regions [49].
Additionally, Figure 4 illustrates the process-induced microstructural heterogeneity of PBT GF30 by presenting the geometry
of the injection-molded tensile specimen, schematic representations of melt-flow conditions, a representative optical micrograph of the reinforced material (PBT GF30) as well as the coordinate system definition used throughout this work, where the longitudinal specimen direction corresponds to the y-axis, the transverse in-plane direction with the x-axis, and the specimen-thickness direction with the z-axis. Therefore, during injection molding, the melt primarily flows along y-axis, which is the longitudinal specimen direction. The longitudinal flow-velocity gradient across the thickness direction z produces a nonuniform shear-rate distribution. Combined with the fountain-flow mechanism at the advancing melt front, these flow conditions result in a layered microstructure with spatially varying fiber orientations [9, 23].
3.2 | Specimen extraction and surface preparation
For the instrumented indentation testing, small sections were extracted from the uniform gage region of the injection-molded tensile specimens, as illustrated in Figure 5. The extracted sections were identified according to their longitudinal position to retain information about their location within the original specimen.
The extracted sections were oriented such that the x-z cross-section, perpendicular to the principal melt-flow direction, formed the surface investigated by instrumented indentation. Consequently, the indentation load was applied parallel to the longitudinal y-direction of the original tensile specimen.
The extracted sections were subsequently embedded and prepared using a sequential metallographic grinding and polishing procedure. Coarse material removal was followed by fine silicon carbide (SiC) grinding up to P2500 [8]. The surfaces were then polished with progressively finer media, including 9 µm and 3 µm diamond suspensions, and finished with a final submicrometer polishing step [42, 56]. After each preparation stage, abrasive residues and material debris were removed to prevent contamination of subsequent polishing steps.
This preparation procedure was chosen to produce a planar and sufficiently smooth cross-section suitable for both contact detection and optical assessment of the resulting indentation imprints. Preliminary measurements on surfaces finished after P2500 grinding were retained for the methodological investigation described in Section 4. Final spatial measurements on PBT GF0 and PBT GF30 were conducted exclusively on fully polished cross-sections.
3.3 | Instrumented indentation system
All indentation experiments were conducted using an instrumented ZHN indentation system supplied by ZwickRoell in collaboration with ASMEC. Figure 6 presents the experimental setup, which includes the instrument and its protective enclosure. Table 1 provides the specifications of the 2 N normal-force unit measuring head.
For the indentation testing the system was equipped with a Berkovich diamond tip. The area function of the indenter and the compliance of the measurement system were calibrated before the experimental investigations. The specimens were mounted with the prepared cross-section perpendicular to the indentation axis. Additionally, thermal drift was addressed by combining environmental shielding with thermal stabilization prior to
5 of 22

FIGURE 4 | Specimen geometry, injection-molding flow conditions, and microstructural heterogeneity of PBT GF30. Left: Geometry of the standardized injection-molded tensile specimens, indicating nominal dimensions and the designated cross-sectional sampling location as specified by DIN EN ISO 527. Center: Schematic diagrams illustrating the principal melt-flow direction (upper) and the velocity distribution with the fountain-flow mechanism at the advancing melt front (lower). Right: Representative optical micrograph of PBT GF30 in the longitudinal y–z plane, highlighting the heterogeneous fiber arrangement resulting from injection molding.
testing. The ZHN indentation system was operated within its thermally and acoustically insulated enclosure, which reduces exposure of the measurement assembly to ambient temperature fluctuations, air currents, and acoustic disturbances. By attenuating changes in the local thermal environment, the enclosure limits temperature-induced dimensional changes within the displacement measurement chain that could otherwise contribute to the recorded indentation depth. Both the specimens and the indentation system were allowed to reach thermal equilibrium in a temperature-controlled laboratory environment for an extended period prior to testing [27, 38]. This thorough thermal stabilization ensured that the thermal drift rate was negligible. Therefore, explicit thermal drift correction was omitted, which is a methodologically established simplification when drift-induced displacement is insignificant compared to the large maximum indentation depths of up to several micrometers examined in this study [40]. However, to eliminate the effects of surface roughness and instrument compliance, a zero-point correction was automatically applied to the raw load-displacement data. The exact point of initial surface contact was determined by fitting a power-law function, that is based on the Hertzian contact model, to the initial segment of the loading curve.
3.4 | Confocal surface and indentation-imprint analysis
Supplementary confocal measurements were performed using a KEYENCE VK-X200 series confocal laser scanning microscope to characterize the effects of surface preparation and the residual
TABLE 1 | Specification of the used 2N normal force unit measuring head provided by ZwickRoell [66] and the official calibration protocol.
| Quantity | Value | Unit |
|---|---|---|
| Maximal test load | N | |
| Minimal test load | approx. 0.2 | mN |
| Digital resolution force | N | |
| Calibration information | Expanded measurement uncertainty of approx. | |
| Maximal displacement | m | |
| Digital resolution displacement | nm | |
| Calibration information | Resolution up to 20 m of 0.9 nm and up to 200 m of 1.1 nm; relative measurement uncertainty of | |
geometry of selected indentation imprints. Representative indentation sites on P2500-ground and polished PBT GF0 surfaces were examined after unloading to identify local surface elevations associated with pile-up and to evaluate the surface topography surrounding the residual indentation cavity.
Confocal measurements were performed at a magnification of 150 x, which provided sufficient spatial resolution to resolve the triangular Berkovich imprint and the surrounding surface topography. Surface profiles across the indentation cavity were analyzed to detect local elevations or depressions relative to the undeformed surface. Surface roughness was quantified using the arithmetic mean roughness and the mean roughness depth
6 of 22
Melt flow direction


4 mm

10 mm
FIGURE 5 | Extraction and preparation of specimens for instrumented indentation. The upper schematic illustrates the extraction of specimen sections from the gage region of an injection-molded tensile specimen and the orientation of the coordinate system relative to the melt-flow direction. The lower photographs show the extraction positions, the separated specimen sections, and the embedded samples prepared for subsequent indentation measurements.
, both calculated from multiple line profiles outside the residual indentation region to ensure that contact detection was not influenced by residual topography [15, 17].
The confocal measurements provided supplementary geometrical assessment and were not used to adjust the projected contact area in the Oliver-Pharr evaluation. Consequently, the profile measurements support the interpretation of the indentation results but do not constitute an independent contact-area correction method. This approach is particularly robust for polymer systems, since rapid and pronounced viscoelastic recovery immediately after indenter unloading significantly alters the residual profile depth, rendering direct area corrections from post-indentation topography measurements highly problematic [17].
4 | Methodological assessment using unreinforced PBT GF0
The initial methodological investigations were conducted on PBT GF0 to assess the influence of experimental and evaluation parameters while limiting the additional variability introduced by the reinforcing phase. First, the effects of indentation spacing and surface preparation were examined, supported by confocal measurements of surface roughness and residual indentation geometry. Subsequently, controlled comparisons were used to assess the influence of maximum load, holding duration, and unloading duration. The sensitivity of the apparent indentation modulus to the unloading fitting interval was evaluated separately. Finally, the influence of loading time on the apparent modulus and the holding-period depth increment was investigated. These investigations informed the selection of a common protocol for the subsequent spatial comparison of PBT GF0 and PBT GF30.

FIGURE 6 | The ZHN instrumented indentation system (ZwickRoel-1/ASMEC) is installed within a thermally and acoustically insulated enclosure for experimental investigations. The enclosure is depicted with its access door open, revealing the indentation instrument and measuring assembly. This enclosure minimizes environmental disturbances during testing.
Therefore, each investigation addresses a specific aspect of the experimental or analytical procedure. Table 2 summarizes these objectives and their role in the subsequent spatial comparison of PBT GF0 and PBT GF30.
4.1 | Minimum indentation spacing
4.1.1 | Experimental setup and measurement procedure
Spatially resolved measurements are required to characterize the variability induced by the microstructural heterogeneity. In order to ensure the independence of these measurements across the surface the minimum distance between consecutive indentation positions was investigated first. Since the minimum distance is directly linked to the indentation area and hence to the indentation depth this analysis was conducted at a maximum load of mN, which equals 87.5% of the maximal operational load of 2000 mN.
Three measurement sequences were performed on PBT GF0, with the point-to-point distance systematically varied from 50 µm to 600 µm in 50 µm increments, as depicted in Figure 7. The investigation employed a loading time of 10 s, a holding time of 10 s, and an unloading time of 4 s as well as a polished measurement surface.
7 of 22
TABLE 2 | Objectives and methodological roles of the conducted preliminary investigations to assess selected influences on the indentation response and support the subsequent comparison of spatially distributed measurements.
| Methodological aspect | Objective | Experimental or analytical approach | Role in the subsequent analysis |
|---|---|---|---|
| Interaction between neighboring indentations (Section 4.1) | Assess whether the measured response depends on the distance from a preceding indentation | Three PBT GF0 sequences with increasing spacing at 1750 mN | Support the selection of the point-to-point spacing |
| Surface condition (Section 4.2) | Assess the influence of preparation on the measured response and residual surface geometry | Comparison of P2500-ground and polished PBT GF0 surfaces, supplemented by confocal measurements | Establish a consistent surface condition and support interpretation of the residual imprints |
| Maximum indentation load (Section 4.3) | Assess the sensitivity of indentation depth and apparent modulus to maximum load | Controlled comparison of 500 and 1000 mN measurements | Distinguish changes in penetration depth from changes in evaluated modulus |
| Holding and unloading durations (Section 4.4) | Assess the influence of temporal loading parameters on the measured response | Controlled comparisons of holding and unloading durations at 500 mN | Support the selection and interpretation of the temporal test conditions |
| Unloading evaluation (Section 4.5) | Assess the dependence of the apparent modulus on the fitting interval | Evaluation of the same curves using broad and initial unloading intervals under three holding/unloading conditions | Identify sensitivity associated with the unloading-curve evaluation |
| Loading duration at final load level of 1750 mN (Section 4.6) | Assess the influence of the preceding ramp on the subsequent holding response | Comparison of four loading durations with fixed maximum load, holding time, and unloading time | Assess the loading-history dependence of and |
4.1.2 | Minimum indentation spacing measurement results
Figure 7 also presents the corresponding contact-depth response. The optical images display the specimen cross-section and three indentation sequences with systematically increasing distances between adjacent positions. The accompanying diagram shows the contact depth as a function of the distance to the preceding indentation. At smaller distances, contact depth demonstrated a marked dependence on indentation spacing, indicating an effect from the deformation field of the previous indentation. While the absolute contact depths varied among the three sequences, their sensitivity to indentation spacing diminished as the distance increased.
With increasing indentation spacing, the contact depth approached a nearly constant value within each measurement sequence. Beyond approximately 400 µm, only minor variations were observed, indicating that the influence of the preceding indentation became negligible compared to the remaining variation within individual sequences. Therefore, a spacing of approximately 400 µm was established as a practical lower limit under the experimental conditions investigated.
4.1.3 | Discussion and spacing definition for subsequent measurements
The spacing investigation demonstrated that, under the experimental conditions, contact depth was largely independent of the distance to the preceding indentation for separations greater than 400 µm. Accordingly, a point-to-point distance of 500 µm was chosen for the final spatial indentation measurements to ensure an additional margin beyond the identified lower limit.
Figure 8 presents a schematic of the measurement grid. The grid comprised a regular arrangement of indentation positions distributed across the polished x-z specimen cross-section, yielding 160 measurement points. The nominal cross-sectional dimensions were 10 mm in the x-direction and 4 mm in the z-direction. A uniform point-to-point distance of 500 µm and a boundary offset of 250 µm were implemented to ensure spatial coverage and to avoid positions adjacent to the specimen edges. The chosen spacing also surpasses commonly reported empirical recommendations, which are typically expressed as multiples of the maximum indentation depth [20, 30, 46, 51]. For the final PBT GF0 measurements, the mean maximum indentation depth was approximately 24.16 µm, resulting in a spacing-to-depth ratio of about 21. However, geometric spacing criteria alone do not eliminate the possibility of mechanical interactions, especially in viscoelastic and heterogeneous polymer systems.
4.2 | Influence of surface preparation and residual indentation geometry
4.2.1 | Surface preparation details and measurement procedure
Maintaining surface roughness below critical thresholds is crucial to avoid initial contact-detection errors and to ensure that local spatial scatter accurately represents material variability rather than artifacts introduced by surface topography [17, 37]. Therefore, in a second step the influence of surface preparation on indentation measurements and residual imprints was investigated by comparing two PBT GF0 specimens, one finished by P2500 grinding and the other subjected to additional polishing. The measurements follow the defined grid of 500 µm × 500 µm with an edge distance of 250 µm, resulting in a total of 160 measurement
8 of 22


FIGURE 7 | Experimental investigation of indentation spacing in PBT GF0 at mN. Top: Optical image of the x-z specimen cross-section showing the locations of the indentation sequences. Middle: Magnified view of three indentation sequences with progressively increasing distances between consecutive indentations. Bottom: Contact depth plotted as a function of the distance to the preceding indentation for the three measurement sequences. The loading, holding, and unloading times were 10 s, 10 s, and 4 s, respectively.
points, as shown in Figure 8. Additionally, the measurement surfaces were analyzed by confocal measurements after the indentation measurements including the surface roughness and the residual indentation geometry.
Because initial contact detection occurs at relatively low loads, surface topography can influence the determination of the displacement origin. To evaluate the influence of surface preparation, both polished and P2500-ground specimens were tested under identical loading conditions, with mN, s, s, and s. The polished and P2500-ground conditions correspond to configurations No. 1 and No. 2, respectively. Configuration No. 1 was used as the reference for comparisons involving surface preparation, maximum load, and unloading duration, while configuration No. 2 served as the reference for the holding-time comparison on P2500-ground surfaces. All apparent indentation moduli were calculated using the unloading interval from 98 to 40 % of . The relevant measurement configurations and results are presented in Table 3. Figure 9 shows representative residual indentation imprints for the two surface conditions.

FIGURE 8 | Schematic arrangement of the spatial indentation grid on the polished x-z cross-section of the injection-molded tensile specimen. A total of 160 indentation positions were arranged in 8 rows and 20 columns, with a nominal point-to-point distance of 500 µm and a boundary offset of 250 µm. The nominal cross-sectional dimensions were 10 mm × 4 mm.


FIGURE 9 | Comparison of the residual indentation geometry on PBT GF0 surfaces with different preparation conditions, obtained using a KEYENCE VK-X200 series confocal laser scanning microscope. Top: Three-dimensional surface topography of a P2500-ground specimen, showing pronounced surface irregularities that complicate the identification of the residual indentation imprint. Bottom: Corresponding three-dimensional surface topography of a polished specimen, allowing clearer identification of the residual Berkovich imprint and the surrounding surface deformation.
9 of 22
TABLE 3 | Comparisons of selected experimental parameters for PBT GF0 are presented. Configuration No. 1 is used as the reference for surface preparation, maximum load, and unloading duration, while configuration No. 2 is the reference for holding-time comparisons on P2500-ground surfaces. All apparent indentation moduli are evaluated using the 98–40 % unloading interval of . The loading-time investigation is conducted separately at mN with a holding duration of 300 s. Values are presented as the mean one standard deviation.
| Comparison | Configuration | [mN] | [s] | [s] | [s] | Surface preparation | Measurement points | [GPa] | [µm] |
|---|---|---|---|---|---|---|---|---|---|
| Reference | No. 1 | 500 | 6 | 20 | 2 | polished | 160 | ||
| Surface preparation | No. 2 | 500 | 6 | 20 | 2 | P2500-ground | 160 | ||
| Load | No. 3 | 1000 | 6 | 20 | 2 | polished | 160 | ||
| Holding time | No. 4 | 500 | 6 | 1 | 2 | P2500-ground | 160 | ||
| No. 5 | 500 | 6 | 10 | 2 | P2500-ground | 160 | |||
| Unloading time | No. 6 | 500 | 6 | 1 | 20 | P2500-ground | 160 | ||
| No. 7 | 500 | 6 | 20 | 20 | polished | 160 | |||
| High-load reference^a | |||||||||
| Loading time | No. 8 | 1750 | 1 | 300 | 4 | polished | 40 | ||
| No. 9 | 1750 | 3 | 300 | 4 | polished | 40 | |||
| No. 10^b | 1750 | 6 | 300 | 4 | polished | 40 | |||
| No. 11 | 1750 | 10 | 300 | 4 | polished | 40 | |||
^aThe 1750 mN measurements were obtained using the independently established final long-hold protocol with a holding time of 300 s, and an unloading time of 4 s. This condition is therefore included as an additional high-load consistency reference and not as a third level of the controlled load comparison.
^bFinal configuration used for the spatially resolved measurements.
4.2.2 | Indentation and confocal measurement results
Although the mechanical response exhibited only minor differences between these methods, substantial variations were observed in surface geometry and the clarity of residual indentation imprints.
Initial confocal measurements showed that the mean roughness-depth values ranged from approximately 1.5 µm to 3.0 µm for the P2500-ground specimen. After polishing, decreased to approximately 0.2 µm to 0.4 µm. The pronounced topographical variations on ground surfaces hindered the distinction between the residual indentation cavity, surrounding pile-up, and undeformed specimen surface. In contrast, polished surfaces allowed for clearer identification of the residual Berkovich imprint and adjacent surface elevations [25].
The residual indentation geometry of polished PBT GF0 was examined in greater detail using confocal laser scanning microscopy. Figure 10 displays a representative three-dimensional surface topography of a residual Berkovich indentation imprint produced at mN, along with the corresponding surface height profile. The results indicate a distinct residual indentation cavity and elevated material adjacent to the imprint, which provides direct experimental evidence of pile-up following unloading.
For the representative polished PBT GF0 imprints examined, residual indentation depths ranged from approximately 2.6 µm to 4.5 µm, while local pile-up heights were approximately 0.2 µm to 0.4 µm. These findings indicate that elastic sink-in alone does not fully account for the residual deformation surrounding the indentation cavity. As a result, the actual projected contact area during indentation may differ from that estimated using the conventional Oliver-Pharr contact-depth relation [42, 5, 16, 54]. Confocal measurements characterize the residual surface geometry after unloading, which may be influenced by subsequent viscoelastic recovery. Therefore, the measured pile-up heights were used for qualitative assessment rather than quantitative correction of the projected contact area.
The effect of surface preparation on the mean apparent indentation modulus was relatively minor. Under otherwise identical experimental conditions, the controlled comparison yielded GPa for the P2500-ground surface (configuration No. 2) and GPa (configuration No. 1) for the polished surface, a difference of 0.04 GPa. The standard deviation decreased from 0.21 GPa to 0.18 GPa (approx. 14%). These results indicate that polishing reduced the variability in the measured indentation modulus while causing only a minor change in its mean value. Similarly, the mean indentation depth changed only from µm to µm. In this case, polishing reduced the standard deviation by approximately 43 %. Thus, the primary benefit of polishing was a reduction in measurement scatter rather than a systematic shift in the mean response [25]. This finding is consistent with the reduced surface roughness and improved identification of residual imprints. All measurement results are summarized in Table 3.
In summary, surface polishing created more favorable conditions for spatially resolved indentation measurements by reducing surface roughness and improving the identification of residual indentation geometry. Because the observed pile-up was not included in a pointwise correction of the projected contact area, the resulting indentation modulus values are consistently interpreted as apparent indentation moduli. This limitation influences the interpretation of their absolute magnitude and should be considered when comparing unreinforced and reinforced material systems.
4.3 | Sensitivity to indentation load
A complementary set of PBT GF0 measurements was conducted to evaluate the sensitivity of the indentation response to maximum load utilizing the already presented measurement setup
10 of 22


FIGURE 10 | Confocal characterization of the residual indentation geometry of polished PBT GF0 following indentation at mN, in accordance with configuration No. 1 in Table 3. Top: Three-dimensional surface topography of a representative Berkovich indentation imprint obtained using a KEYENCE VK-X200 series confocal laser scanning microscope. The indicated line defines the position of the profile evaluation. Bottom: Corresponding surface height profile illustrating the residual indentation cavity and adjacent elevated material regions associated with pile-up.
with a total of 160 measurement points where the maximum load was increased from 500 mN (configuration No. 1) to 1000 mN (configuration No. 3).
The most significant response to an increase in the maximum indentation load was observed in the indentation depth. Under otherwise identical conditions, increasing from 500 mN to 1000 mN raised the mean indentation depth from 10.95 µm to 15.58 µm (approximately 42%), as expected. In contrast, the apparent indentation modulus changed only from 3.00 GPa to 2.88 GPa, a difference of approximately 4%. Thus, in this controlled comparison, the increase in maximum load mainly affected the magnitude of the indentation rather than the local stiffness evaluated.
The associated standard deviations corroborate this interpretation. For , the standard deviation increased moderately from 0.18 GPa to 0.22 GPa. For indentation depth, the increase from 0.25 µm to 0.44 µm reflects the larger absolute displacement at higher indentation load. Therefore, increased penetration was accompanied by greater absolute depth scatter, while the mean apparent indentation modulus remained nearly unchanged.
This outcome confirms that the apparent modulus is largely independent of peak force within this load range. This load independence is physically expected for geometrically self-similar indenters (such as the Berkovich tip) once the indentation depth is sufficiently large to overcome tip blunting and near-surface artifacts, typically occurring at contact depths exceeding 100 nm [26, 41]. However, these results do not demonstrate complete load independence.
4.4 | Sensitivity to holding and unloading duration
The effects of holding and unloading durations were examined using PBT GF0 measurements at mN with a constant loading duration of 6 s. For the holding-time comparison, configurations No. 4 and No. 5, with holding durations of 1 s and 10 s, respectively, were compared to configuration No. 2, which used a holding duration of 20 s. All three configurations were performed on P2500-ground surfaces with an unloading duration of 2 s. The influence of unloading duration was assessed through two complementary comparisons: configurations No. 4 and No. 6 on P2500-ground surfaces with a holding duration of 1 s, and configurations No. 1 and No. 7 on polished surfaces with a holding duration of 20 s. The results are presented in Table 3.
An increase in holding duration from 1 s to 20 s resulted in a rise in the mean apparent indentation modulus from 2.84 GPa to 2.96 GPa, representing approximately 4.2 %. At the intermediate holding duration of 10 s, the mean apparent indentation modulus was 2.95 GPa. The corresponding mean contact depths were 10.74 µm, 11.17 µm, and 11.25 µm for holding durations of 1 s, 10 s, and 20 s, respectively. These findings demonstrate a moderate variation in the indentation response with holding duration. However, as the compared configurations originated from different preliminary measurement series, the observed differences should be interpreted descriptively rather than attributed solely to the holding-time effect.
For P2500-ground PBT GF0, extending the unloading duration from 2 s (No. 4) to 20 s (No. 6) at a fixed holding duration of 1 s increased the mean apparent indentation modulus from 2.84 GPa to 3.01 GPa, an increase of approximately 6.0 %. The mean contact depth also increased slightly from 10.74 µm to 10.85 µm. Conversely, on polished surfaces at a holding duration of 20 s (No. 1 and No. 7), the mean apparent indentation modulus decreased from 3.00 GPa to 2.75 GPa, a reduction of approximately 8.3 %. The associated mean contact depth increased from 10.95 µm to 11.09 µm.
These contrasting trends indicate that the apparent indentation modulus displays varying sensitivities to unloading duration under the tested conditions. Notably, differences in preceding holding duration and surface preparation between the two comparisons preclude unambiguous attribution of the observed trends to a single experimental parameter. Continued viscoelastic deformation and recovery during unloading may also affect the unloading curvature and the resulting contact stiffness [5, 17, 21]. These results underscore the necessity of maintaining consistent temporal testing and evaluation conditions when comparing indentation responses.
11 of 22
4.5 | Influence of the unloading evaluation interval
The sensitivity of the apparent indentation modulus to the unloading fitting interval was assessed to quantify the effect of ongoing viscoelastic deformation immediately after peak load [17, 21]. This evaluation involved analyzing identical force-displacement responses over the 98–40 % and 100–90 % intervals of . Configurations No. 4, No. 5 and No. 6 were included in the analysis, all performed on P2500-ground PBT GF0 surfaces at mN. The corresponding mean values and standard deviations are provided in Table 4.
TABLE 4 | Influence of the unloading fitting interval on the apparent indentation modulus of PBT GF0 at mN. All measurements were performed on P2500-ground surfaces. Values are reported as mean one standard deviation.
| Configuration | [s] | [s] | [GPa] | [GPa] |
|---|---|---|---|---|
| No. 4 | 1 | 2 | 2.84 ± 0.23 | 3.00 ± 0.25 |
| No. 5 | 10 | 2 | 2.95 ± 0.22 | 2.93 ± 0.22 |
| No. 6 | 1 | 20 | 3.01 ± 0.20 | 3.69 ± 0.31 |
A pronounced dependence on the fitting interval was observed when a short holding period was combined with slow unloading. For s and s, restricting the evaluation from the broader 98–40 % interval to the initial 100–90 % unloading interval increased the mean apparent indentation modulus from 3.01 GPa to 3.69 GPa, corresponding to approximately 22.6 %. Under these conditions, the brief holding phase induces substantial creep activity within the material. During the subsequent slow unloading, this persistent forward creep competes with elastic recovery. This competition artificially steepens the initial unloading slope and results in a significant overestimation of the calculated stiffness [11, 29, 40]. Consequently, the local curvature immediately after the peak load does not accurately represent the overall unloading response in such cases. These results highlight the necessity of optimizing fitting windows for viscoelastic polymer systems [52].
The discrepancy between fitting intervals was greatly reduced when the unloading duration was shortened to 2 s. Additionally, after a holding period of 10 s and rapid unloading, both fitting intervals yielded nearly identical mean values of approximately 2.94 GPa. These results indicate that the sensitivity of the initial unloading response decreases when the material experiences additional time-dependent deformation before unloading and when the subsequent load reduction is rapid. This confirms that sufficiently high unloading rates effectively minimize the history-dependent viscoelastic contribution to contact stiffness [60].
Based on this comparison, the broad fitting interval (40–98 %) was selected for the final evaluation, consistent with the established mesoscale indentation protocols for the SFRC. This interval reduces the influence of localized curvature immediately after the holding segment and provides a consistent and robust evaluation basis for all spatial measurements. Incorporating a substantially longer holding period of 300 s in the final protocol further decreases the displacement rate at the onset of unloading to negligible levels, effectively eliminating residual viscoelastic unloading artifacts.
Comparable sensitivity was also detected during the unloading phase. Short holding periods combined with slow unloading resulted in a pronounced dependence of on the chosen fitting interval. This dependence was reduced when additional time-dependent deformation was allowed before unloading, allowing the creep rate to decrease, and when the subsequent unloading segment was shortened [17, 21, 40].
4.6 | Influence of loading time at high load
The final assessment focuses on the loading time. Since the loading time is directly related to viscoelastic behavior, here the identical load level from the spatially resolved measurements of mN with an extended holding period of 300 s is used. This high-load condition and extended holding period of 300 s are consistent with established microscale testing protocols for characterizing process-induced local viscoelastic fluctuations in SFRC. The high load was selected to ensure that the resulting displacement produced a pronounced and stable time-dependent signal during the holding segment. Thus, the final force selection represents a compromise among displacement resolution, spatial sampling scale, and the geometrical constraints imposed by increasing indentation size, allowing the indentation volume to act as a representative mesoscale sampling element [16].
4.6.1 | High load assessment
An independently obtained high-load dataset provides an additional reference for the sensitivity of the apparent indentation modulus to the indentation force. At mN, the final long-hold protocol yielded an apparent indentation modulus of GPa and a maximum indentation depth of µm. The apparent indentation modulus therefore remained within the range observed for the controlled measurements 500 mN and 1000 mN, despite the substantially larger indentation depth, indicating the absence of pronounced effects of indentation size in this depth regime [42, 60].
However, the 1750 mN condition was conducted with a substantially longer holding period of 300 s and a different unloading duration. Therefore, it does not represent a third level of the controlled load comparison. Instead, this result serves as an independent consistency reference, indicating that the apparent indentation modulus remains of the same order throughout the extended load range investigated in this study. The higher load was subsequently retained in the final protocol because the associated increase in indentation depth provides a sufficiently pronounced displacement signal for characterizing the time-dependent indentation response.
4.6.2 | Loading time assessment
The effect of the loading ramp was examined independently at mN. Loading durations of 1 s, 3 s, 6 s, and 10 s were assessed, with holding and unloading durations fixed at 300 s and 4 s, respectively. For each loading duration, 40 indentation positions were analyzed.
Table 5 presents the apparent indentation modulus , the absolute indentation creep depth increment , and the relative indentation creep for the four investigated loading durations.
12 of 22
The relative indentation creep, determined according to Eq. (8), serves as an additional measure of the time-dependent response by normalizing the holding-period displacement increment with respect to the indentation depth at the beginning of the holding period. All quantities are reported as mean values with corresponding standard deviations.
TABLE 5 | Influence of loading duration on the apparent indentation modulus, absolute indentation creep depth increment, and relative indentation creep of PBT GF0 at , , and . Each configuration comprises 40 indentation positions. Values are reported as mean one standard deviation.
| Config. | [s] | [GPa] | [µm] | [%] |
|---|---|---|---|---|
| No. 8 | 1 | |||
| No. 9 | 3 | |||
| No. 10 | 6 | |||
| No. 11 | 10 |
The apparent indentation modulus remained within a narrow range of 2.89 GPa to 3.03 GPa, with no monotonic dependence on loading duration observed. Therefore, variation in the loading ramp influenced the stiffness-related parameter significantly less (appr. 4.8 % relative to the lowest mean value) than the subsequent time-dependent displacement, confirming that the exceptionally long hold duration of 300 s successfully allowed the viscoelastic deformation rate to diminish prior to unloading, thereby yielding drift-insensitive contact stiffness evaluations [17, 42].
In contrast, both the absolute indentation creep depth increment and the relative indentation creep demonstrated a strong dependence on the preceding loading duration. The highest mean creep increment, approximately 2.88 µm, was recorded after the 1 s loading ramp, while the lowest value, approximately 1.97 µm, was measured after 10 s. This represents a reduction of approximately 31.6 %. A similar tendency was observed for , which decreased from 13.44 % to 9.14 % between the shortest and longest loading durations, amounting to a reduction of approximately 32.0 %. Although the intermediate values of both creep measures did not decrease monotonically, the overall trends indicate a significant influence of the preceding loading duration on the time-dependent indentation response.
In summary, varying the loading duration between 1 s and 10 s resulted in moderate, non-monotonic differences in , while substantially larger variations were observed in both and . This behavior can be explained by the definition , where denotes the indentation depth at the beginning of the holding period [58]. A longer loading duration permits a greater proportion of time-dependent deformation to accumulate before is reached. Because this deformation is already included in , it does not contribute to the subsequent holding-period increment [5, 8, 63]. The observed reduction in demonstrates that the relative indentation depth increment is also influenced by the preceding loading history. Therefore, meaningful comparisons of time-dependent indentation responses require identical loading and holding durations.
4.7 | Definition of the final indentation protocol
Preliminary investigations demonstrate that spatially resolved indentation of PBT requires a clear distinction between parameters affecting deformation amplitude and those influencing the evaluation of the unloading response. This distinction is particularly important for viscoelastic polymers, since deformation persists beyond the maximum indentation load and continuously alters the stress and displacement fields below the indenter tip [5, 13, 17].
Following the comprehensive methodological investigations, a unified indentation protocol was established for the spatial comparison of PBT GF0 and PBT GF30. The selected parameters are presented in Table 6.
TABLE 6 | Final indentation protocol used for the spatially resolved characterization of PBT GF0 and PBT GF30.
| Parameter | Selected value |
|---|---|
| Maximum indentation load | 1750 mN |
| Loading time | 6 s |
| Holding time | 300 s |
| Unloading time | 4 s |
| Point-to-point spacing | 500 µm |
| Nominal boundary offset | 250 µm |
| Number of indentation positions | 160 |
| Unloading fitting interval | 98–40 % of |
| Surface condition | polished |
Each parameter was chosen to address specific sources of experimental uncertainty. The selected spacing exceeds the experimentally determined minimum distance of approximately 400 µm, and the polished surface minimizes disturbances caused by surface topography. The loading time ensures a reproducible transition to peak load without unduly prolonging the period during which time-dependent deformation may accumulate prior to the holding segment.
The high-load condition and extended holding period of 300 s are consistent with established microscale testing protocols for characterizing process-induced local viscoelastic fluctuations in SFRC. The high load was selected to ensure that the resulting displacement produced a pronounced and stable time-dependent signal during the holding segment. Thus, the final force selection represents a compromise among displacement resolution, spatial sampling scale, and the geometrical constraints imposed by increasing indentation size, allowing the indentation volume to act as a representative mesoscale sampling element [16].
An extended holding period was implemented to generate a pronounced time-dependent displacement signal and to decrease the displacement rate prior to unloading. The subsequent 4 s unloading segment restricts the duration in which creep and recovery may affect the stiffness evaluation. The preliminary comparison supports limiting the duration of unloading but does not directly establish 4 s as an optimal value under the final testing conditions. Accordingly, this duration is treated as a fixed protocol parameter rather than an independently optimized setting. Additionally, the (40–98 %) fitting interval further reduces sensitivity to local curvature immediately after the transition from holding to unloading.
13 of 22
The loading-time investigation does not support the existence of a universal ramp duration beyond which indentation creep becomes independent of loading history. Instead, an identical loading ramp is necessary when comparing absolute creep increments between material systems. A loading duration of 6 s was chosen for the final protocol due to its minimal force overshoot, relatively low response scatter, and sufficiently rapid transition into the prolonged holding segment, representing a robust balance between machine dynamics and minimizing early viscoelastic losses [58]. Therefore, the final protocol, which incorporates a 300 s holding period, 4 s unloading duration, and a 98–40 % fitting interval, establishes a consistent evaluation procedure and effectively reduces sensitivity to transient viscoelastic unloading artifacts near the hold-to-unload transition. This approach prevents the occurrence of "nose" anomalies and artificial stiffness inflation [11, 28, 40].
Even though the resulting indentation depth observed for a selected holding period of 300 s in combination with a larger load is significantly deeper than for a holding time of 10 s, the resulting indentation depth still meets the reported empirical recommendations as multiples of the maximum indentation depth as documented in [20, 30, 46, 51]. Therefore, the same measurement grid of 160 points with a point-to-point distance of 500 µm is used for both PBT GF0 and PBT GF30 to ensure comparable measurement conditions. Additionally, the selected spacing should be regarded as an experimentally motivated criterion rather than a universally verified, interaction-free limit for all subsequent measurements. The protocol, specimen preparation, measurement grid, and evaluation procedure were consistently applied to both material systems. Consequently, systematic differences in the resulting spatial distributions can be attributed primarily to variations in local material response rather than to alterations in the experimental procedure.
5 | Spatially resolved indentation response of PBT GF0 and PBT GF30
5.1 | Procedure of the spatially resolved indentation measurement
After these preliminary investigations, spatially resolved measurements were performed using the final indentation protocol as given in Table 6 that aims to minimize viscoelastic recovery artifacts during the subsequent unloading stage, which would otherwise distort the indentation modulus evaluation [5, 17].
Following established mesoscale mapping strategies for SFRC [49], a regular spatial grid containing 160 indentation positions was applied in each investigated cross-section, as shown in Figure 8. The complete force–displacement response was continuously recorded during loading, holding, and unloading. For the final evaluation, the unloading curve was approximated over the range from approximately 98 % to 40 % of , and the same evaluation settings were applied to all material systems. The resulting data were used to characterize the spatial indentation response and its statistical properties as summarized in Table 7.
5.2 | Overall load–displacement response
The final indentation protocol yielded distinct experimental force–displacement responses for the unreinforced and reinforced material systems. Figure 11 presents the superimposed force–displacement curves obtained at the investigated indentation positions for PBT GF0 and PBT GF30. Each curve comprises the loading segment, the additional penetration during the constant-load holding period, and the subsequent unloading response. The comparison illustrates differences in the overall indentation response and its local variability between the two material systems.
(a) PBT GF0

(b) PBT GF30

FIGURE 11 | Experimental force–displacement responses for (a) PBT GF0 and (b) PBT GF30 were obtained using the final indentation protocol with mN, s, s, and s. The superimposed curves demonstrate the variation in indentation response across the investigated measurement positions.
PBT GF0 exhibited a mean maximum indentation depth of approximately 24.16 µm with a standard deviation of 0.91 µm. In contrast, PBT GF30 demonstrated a lower mean maximum depth of approximately 18.93 µm and a standard deviation of 0.94 µm. This reduced penetration in the reinforced material aligns with its increased local resistance to indentation.
A time-dependent increase in indentation depth occurred during the 300s holding segment for both materials. However, the magnitude and spatial variability of this increase differed substantially between PBT GF0 and PBT GF30, as discussed in the following sections.
14 of 22
TABLE 7 | Objectives and evaluation approaches of the spatially resolved indentation investigations conducted on PBT GF0 and PBT GF30 at the mesoscale.
| Methodological aspect | Objective | Experimental or analytical approach | Resulting information |
|---|---|---|---|
| Spatial material response | Compare the local indentation response of unreinforced and reinforced PBT | Application of the predefined protocol to polished PBT GF0 and PBT GF30 cross-sections | Obtain spatially distributed stiffness-related and creep-related response quantities |
| Statistical description | Distinguish differences in mean response from differences in relative scatter | Evaluation of means, standard deviations, and CoV | Quantify the observed differences between the final spatial datasets |
5.3 | Spatial distribution of the apparent indentation modulus
Figure 12 shows the spatial distribution of the apparent indentation modulus across the investigated x-z cross-sections. Retaining the coordinates of the measurement positions during evaluation enabled representation of the local response over the entire measured cross-sectional area.
PBT GF0 exhibited a relatively narrow spatial distribution of . Most indentation positions fell within a limited range around the mean response, which aligns with the absence of a discrete reinforcement phase. The remaining spatial scatter can be attributed to local polymer morphology, processing-related variations, and residual experimental uncertainty.
In contrast, PBT GF30 displayed a substantially broader local modulus distribution. Regions with both low and high values were observed throughout the investigated cross-section. At the indentation scale, the sampled material volume may contain varying proportions and orientations of polymer matrix, glass fibers, and fiber–matrix transition regions. Therefore, the measured modulus reflects the apparent local response of the heterogeneous material volume rather than a phase-specific material constant.
The reinforced material thus exhibited both an increased mean local stiffness and a more heterogeneous spatial stiffness distribution. This finding is consistent with the process-induced microstructure of injection-molded SFRCs, for which local fiber content and fiber orientation vary throughout the cross-section [49].
5.4 | Spatial distribution of indentation creep
Figure 13 presents the spatial distributions of the indentation creep depth increment. The parameter denotes the additional penetration accumulated during the 300 s holding period at constant .
PBT GF0 exhibited a comparatively uniform spatial response. Despite some local deviations, the creep increment remained concentrated within a relatively narrow range across most of the cross-section. The unreinforced polymer thus served as a reference for the inherent variability of the matrix-dominated indentation response.
In the case of PBT GF30, the mean creep increment was lower, but the local scatter was considerably greater. Distinct regions with relatively small and large were observed within the same cross-section. Therefore, short-fiber reinforcement did not uniformly reduce the time-dependent indentation response. Instead, the magnitude of the local deformation increment depended on
the heterogeneous mechanical constraints imposed by the surrounding microstructure.
The spatial variation in creep response complements the corresponding modulus distribution. These two maps demonstrate that reinforcement-induced heterogeneity influences both the stiffness-related unloading response and the time-dependent displacement accumulated under sustained indentation load.
5.5 | Statistical comparison of PBT GF0 and PBT GF30
Quantitative statistics for the spatial distributions are presented in Tables 8, 9, and 10. All 160 indentation positions were retained for PBT GF0. For PBT GF30, one position was excluded due to unstable initial contact detection, which resulted in an invalid force–displacement response, leaving 159 valid measurements.
TABLE 8 | Statistical summary of the apparent indentation modulus obtained for PBT GF0 and PBT GF30.
| Material | Valid points [–] | Mean [GPa] | Standard deviation [GPa] | CoV [%] | Range [GPa] |
|---|---|---|---|---|---|
| PBT GF0 | 160 | 2.91 | 0.197 | 6.77 | 2.2–3.1 |
| PBT GF30 | 159 | 6.65 | 0.597 | 8.97 | 5.0–8.1 |
The mean apparent indentation modulus increased from 2.91 GPa for PBT GF0 to 6.65 GPa for PBT GF30. Thus, incorporation of short glass fibers increased the mean local stiffness response by approximately 129 % under the selected indentation conditions.
The absolute scatter also increased, as indicated by the standard deviation rising from 0.197 GPa to 0.597 GPa. Given the substantial difference in mean modulus between the two materials, the CoV offers a more suitable metric for comparing relative variability. The CoV increased from 6.77 % for PBT GF0 to 8.97 % for PBT GF30, representing a relative scatter increase of approximately 32.5 %.
The mean indentation creep depth showed the opposite trend. PBT GF0 yielded a mean value of 2.36 µm, while PBT GF30 exhibited a lower mean value of 1.91 µm. Consequently, the mean displacement accumulated during the holding period decreased by approximately 19 % after reinforcement.
Despite this reduction in the mean response, the spatial variability increased substantially. The standard deviation increased from 0.161 µm for PBT GF0 to 0.233 µm for PBT GF30, while the
15 of 22
(a) PBT GF0

(b) PBT GF30

FIGURE 12 | Spatial distribution of the apparent indentation modulus obtained from the unloading response of instrumented indentation measurements on the x-z cross-sections of (a) PBT GF0 and (b) PBT GF30, using the final indentation protocol with mN and s.
(a) PBT GF0

(b) PBT GF30

FIGURE 13 | Spatial distribution of the absolute indentation creep depth increment obtained during the 300 s holding period at mN across the x-z cross-sections of (a) PBT GF0 and (b) PBT GF30.
CoV increased from 6.83 % to 12.17 %. The corresponding relative increase in the CoV was approximately 78 %.
In addition to the absolute indentation creep depth increment, the relative indentation creep was evaluated using Equation (8). Table 10 presents the corresponding statistical results.
The mean relative indentation creep increased slightly from 10.84 % for PBT GF0 to 11.29 % for PBT GF30, representing an increase of approximately 4.2 % relative to the unreinforced material. In contrast, spatial variability increased markedly. The standard deviation increased from 0.458 to 1.515 percentage points, and the corresponding CoV increased from 4.23 % to 13.42 %. These results suggest that short-fiber reinforcement reduced the mean absolute indentation creep depth increment but did not decrease the mean relative indentation creep under
16 of 22
TABLE 9 | Statistical summary of the indentation creep depth increment obtained for PBT GF0 and PBT GF30.
| Material | Valid points [-] | Mean [µm] | Standard deviation [µm] | CoV [%] | Range [µm] |
|---|---|---|---|---|---|
| PBT GF0 | 160 | 2.36 | 0.161 | 6.83 | 2.19–3.22 |
| PBT GF30 | 159 | 1.91 | 0.233 | 12.17 | 1.47–2.60 |
TABLE 10 | Statistical summary of the relative indentation creep obtained for PBT GF0 and PBT GF30.
| Material | Valid points [-] | Mean [%] | Standard deviation [%] | CoV [%] | Range [%] |
|---|---|---|---|---|---|
| PBT GF0 | 160 | 10.84 | 0.458 | 4.23 | 9.4–12.8 |
| PBT GF30 | 159 | 11.30 | 1.518 | 13.43 | 8.3–16.6 |
the tested loading conditions. Moreover, the increased CoV indicates substantially greater relative variability in the normalized time-dependent indentation response of PBT GF30.
The combined statistical results indicate that short-fiber reinforcement increases the mean apparent indentation modulus and reduces the mean absolute indentation creep depth increment. In contrast, the mean relative indentation creep shows a slight increase. Additionally, the relative spatial variability increases for all three investigated quantities, suggesting a more heterogeneous local indentation response in PBT GF30.
5.6 | Integrated discussion and limitations
5.6.1 | Interpretation of the apparent indentation modulus
Interpreting the absolute magnitude of the indentation modulus requires caution, as the local contact response fundamentally differs from that of a homogeneous uniaxial tensile state. The indentation stress field is multiaxial, the sampled material volume is limited, and both plastic and time-dependent deformation may occur throughout the loading cycle [4, 5]. Additionally, the heterogeneous PBT GF30 material exhibits locally varying fiber orientations and phase fractions within the indentation-affected region.
Confocal measurements confirmed the presence of pile-up around representative polished PBT GF0 indentation imprints. Because the conventional Oliver-Pharr procedure estimates the projected contact area from the contact depth using a sink-in-based model, uncorrected pile-up may cause the actual contact area to exceed the calculated value. As a result, the measured indentation modulus is overestimated [3, 43, 60, 64]. This conclusion is based on standard linear elastic tensile tests performed on PBT GF0 where a Young's modulus of 2.67 GPa with a standard deviation of 0.30 GPa was obtained.
No pointwise pile-up correction was available for complete spatial measurement grids. Therefore, is interpreted as an apparent indentation modulus throughout this study and should not be considered an exact intrinsic Young's modulus of either the matrix or the composite. This distinction is especially important for PBT GF30, where individual indentation positions sample different local fiber-matrix configurations that introduce
localized structural constraints and alter plastic-zone development [16, 57].
However, the absence of an explicit pile-up correction does not exclude the comparative analysis conducted in this study. PBT GF0 and PBT GF30 were prepared, tested, and evaluated using identical experimental procedures. Consequently, the observed differences offer a consistent measure of the reinforcement effect at the investigated indentation scale, although the absolute values remain subject to the limitations of the contact-area approximation.
5.6.2 | Effect of short-fiber reinforcement on mean local response
Spatial measurements demonstrate a pronounced reinforcement effect in both stiffness-related and time-dependent indentation parameters. The mean apparent indentation modulus increased from 2.91 GPa to 6.65 GPa, while the mean maximum indentation depth decreased from approximately 24.16 µm to 18.93 µm. These results indicate enhanced local resistance to deformation after the incorporation of short glass fibers, consistent with the expected mesoscale stiffening of SFRC [32, 48].
The mean creep increment also decreased from 2.36 µm to 1.91 µm. Thus, the reinforcement increased resistance to initial indentation and reduced additional penetration under sustained load. This behavior is consistent with the mechanical constraint imposed by the relatively stiff reinforcement on the deformation of the surrounding polymer matrix, which restricts the development and propagation of the plastic zone beneath the indenter [7, 16, 36].
The absolute indentation creep depth is not an intrinsic creep material parameter. Its magnitude depends on indentation force, loading ramp, holding duration, initial indentation depth, indenter geometry, and local mechanical constraint. Consequently, this quantity serves as a comparative local measure of the time-dependent response under the specific experimental protocol employed in this study [4, 13, 63].
The selected examples show that a higher apparent indentation modulus does not necessarily coincide with a smaller absolute holding-period depth increment , which meets the theoretical definition of these two quantities. The apparent modulus is obtained from the unloading response, which reflects instantaneous elastic recovery. In contrast, is determined by the displacement accumulated during the preceding holding period, which is governed by transient viscoelastic and viscoplastic flow [4, 40]. These two quantities assess distinct aspects of the local material response, although both are affected by the surrounding microstructure.
5.6.3 | Reinforcement-induced spatial variability
A principal outcome of the spatial analysis is that short-fiber reinforcement influences both the mean response and its relative variability. For the apparent indentation modulus , the CoV increased from 6.77 % for PBT GF0 to 8.97 % for PBT GF30. This increase of approximately 32.5 % demonstrates that the reinforced material exhibits a broader relative distribution of local stiffness values.
This effect is even more pronounced for the time-dependent indentation response. The CoV of increased from 6.83 % to
17 of 22
12.17 %, representing an increase of approximately 78 % in relative scatter. Although reinforcement reduces the mean creep displacement, the magnitude of this reduction varies substantially across local material regions.
The relative indentation creep provides an additional perspective on the time-dependent indentation response by incorporating the indentation depth at the start of the holding period. The mean value increased slightly from 10.84 % for PBT GF0 to 11.29 % for PBT GF30, which represents an increase of approximately 4.2 %. In contrast, CoV increased substantially from 4.23 % to 13.42 %, corresponding to an increase of approximately 217 % in relative scatter. Although short-fiber reinforcement reduced the mean absolute indentation creep depth increment , the normalized creep response did not exhibit a comparable reduction. This distinction highlights the impact of varying initial indentation depths and underscores the importance of considering both absolute and relative creep measures when comparing heterogeneous material systems.
The comparatively narrow distributions observed for PBT GF0 serve as a reference for the combined effects of matrix heterogeneity and experimental scatter. In contrast, the increased variability in PBT GF30 is attributable to the heterogeneous microstructure introduced by short glass fibers. Individual indentation sites may exhibit differences in local fiber fraction, fiber orientation, matrix-dominated regions, and fiber-matrix interfaces. These localized variations and the resulting boundary-interaction effects, often referred to as "fiber bias" or "fiber constraint" effects, have been shown to broaden the statistical distribution of both modulus and hardness measurements in fiber-reinforced systems [16, 22, 35]. Additionally, the injection-molding process produces systematic variations in reinforcement morphology across the specimen cross-section.
To further illustrate the microstructural heterogeneity underlying the spatially varying indentation response, Figure 14 presents representative post-indentation micrographs from four selected PBT GF30 measurement positions. The images reveal distinct local fiber-matrix configurations, characterized by variations in the number, spatial arrangement, and proximity of visible glass-fiber cross-sections relative to the residual Berkovich imprints. These findings qualitatively demonstrate the heterogeneous material configurations encountered during indentation. The corresponding measurement coordinates and local indentation quantities are summarized in Table 11, which enables identification of the selected positions in the spatial distributions shown in Figures 12 and 13.
TABLE 11 | Measurement coordinates and indentation values for the representative PBT GF30 indentation sites are presented as shown in Figure 14. These coordinates align with the spatial positions depicted in Figures 12 and 13.
| Panel | x [mm] | z [mm] | [GPa] | [µm] | [µm] |
|---|---|---|---|---|---|
| a) | 6.25 | 1.75 | 5.6 | 1.695 | 18.561 |
| b) | 3.25 | 0.75 | 6.9 | 1.592 | 17.331 |
| c) | 6.25 | 0.75 | 7.4 | 1.828 | 15.154 |
| d) | 1.25 | 2.25 | 7.9 | 2.402 | 15.611 |
The corresponding apparent indentation moduli at the selected locations ranged from 5.6 GPa at position (a) to 7.9 GPa at position (d). In contrast, the absolute indentation creep depth increments varied between 1.592 µm and 2.402 µm. Notably, position (d) exhibited both the highest indentation modulus and the largest creep increment among the four locations, demonstrating that these quantities are not necessarily inversely related. While the micrographs reveal differences in the visible local fiber configurations, the measured indentation response is influenced by the three-dimensional heterogeneous material volume beneath the indenter. Therefore, these observations are interpreted qualitatively and do not establish a quantitative relationship between the visible fiber distribution and the local mechanical response.
A single deterministic value does not adequately capture the full range of local indentation responses in PBT GF30. Employing large arrays of indentations (grid indentation) with statistical descriptors enables a more comprehensive characterization of heterogeneous materials. Although statistical grid indentation was initially developed for the deconvolution and identification of discrete, homogeneous phase properties [6, 62], the present study applies this spatial mapping technique to characterize the continuous statistical distribution of mesoscale apparent properties. Spatial maps and related statistical descriptors, such as the CoV and probability density distributions, provide essential insights into the magnitude and variability of the local composite response [50]. These data are especially important when local microstructural heterogeneity is incorporated into probabilistic material models.
However, the current measurements alone do not provide a comprehensive stochastic random-field characterization. Such a representation requires quantification of the spatial dependence between measurement locations, for example, through covariance or autocorrelation functions and corresponding correlation lengths. The present results establish experimental marginal statistics and spatial response maps that can serve as input for, or be supplemented by, subsequent spatial stochastic analyses.
6 | Conclusions
A combined methodological and spatially resolved indentation approach was employed to characterize the apparent local stiffness and time-dependent indentation response of injection-molded PBT GF0 and PBT GF30. The methodological analysis identified experimental conditions that allow differentiation between local response variability and significant measurement-parameter effects.
The spacing analysis demonstrated that the effect of a preceding indentation became negligible at distances of approximately 400 µm under a maximum load of 1750 mN. Consequently, a conservative spacing of 500 µm was selected for the final spatial grid. Additionally, polishing reduced the mean roughness depth from approximately 1.5 µm–3.0 µm for P2500-ground surfaces to approximately 0.2 µm–0.4 µm, enabling reliable identification of the residual indentation geometry and surrounding pile-up.
The preliminary load comparison for PBT GF0 demonstrated that increasing the maximum load from 500 mN to 1000 mN resulted in a substantial increase in calculated contact depth, whereas the corresponding change in apparent indentation modulus remained moderate. At 500 mN, extending the holding duration
18 of 22 a)
b)

c)
d)

FIGURE 14 | Representative post-indentation confocal micrographs of four Berkovich imprints in PBT GF30. Subfigures a)-d) show individual indentation sites with distinct local fiber-matrix configurations. Differences are visible in the number, spatial arrangement, and proximity of glass-fiber cross-sections relative to the residual imprints. The micrographs qualitatively illustrate variations in the local surface microstructure associated with the mesoscale material volumes involved in the indentation response. The scale bar in each micrograph corresponds to 50 µm.
from 1 s to 20 s led to a moderate increase in the mean apparent indentation modulus from 2.84 GPa to 2.96 GPa. These findings, however, were derived from separate preliminary measurement series. The influence of unloading duration varied depending on the specific testing conditions, and the choice of unloading fitting interval substantially affected the evaluated modulus under certain circumstances.
Varying the loading duration between 1 s and 10 s produced apparent indentation moduli ranging from approximately 2.9 GPa to 3.0 GPa, with no monotonic dependence on loading time. However, the subsequent creep depth varied substantially because different fractions of the time-dependent deformation accumulated during the preceding loading ramp. These findings indicate that the absolute indentation creep quantities are directly comparable only when an identical temporal loading protocol is applied.
Based on the methodological assessment, a final protocol consisting of mN, s, s, and s was implemented for the spatial measurement grids in PBT GF0
and PBT GF30. The unloading response was consistently evaluated on the 98–40 % interval of .
The mean apparent indentation modulus increased from 2.91 GPa for PBT GF0 to 6.65 GPa for PBT GF30, representing an increase of approximately 129 %. In contrast, the mean creep depth decreased from 2.36 µm to 1.91 µm, a reduction of approximately 19 %. Thus, short-fiber reinforcement enhanced the local resistance to both initial and sustained indentation deformation. Simultaneously, the relative spatial variability increased. The CoV of increased from 6.77 % to 8.97 %, while the CoV of increased from 6.83 % to 12.17 %. Therefore, reinforcement reduced the mean time-dependent indentation displacement, but resulted in a substantially more heterogeneous local response.
Confocal measurements confirmed local pile-up around representative PBT indentation imprints. As no pointwise contact-area correction was applied, the reported modulus values represent apparent indentation moduli obtained using a consistent
19 of 22
Oliver-Pharr evaluation rather than exact intrinsic Young's moduli. Within this limitation, the established methodology offers a consistent experimental basis for quantifying both the mean local response and the spatial variability of SFRCs.
Author Contributions
Eduard Klatt: Conceptualization, Methodology, Software, Data Curation, Investigation, Validation, Formal analysis, Visualization, Writing - Original Draft, Writing - Review & Editing
Natalie Rauter: Conceptualization, Methodology, Validation, Supervision, Project administration, Resources, Writing - Original Draft, Writing - Review & Editing
Conflicts of Interest
The authors declare no conflicts of interest.
Data Availability Statement
The data that support the findings of this study are openly available in Zenodo at 10.5281/zenodo.23766180.
References
-
S. G. Advani and III Tucker, C. L. The use of tensors to describe and predict fiber orientation in short fiber composites. Journal of Rheology, 31(8):751–784, 1987. ISSN 0148-6055. doi: 10.1122/1.549945. URL https://doi.org/10.1122/1.549945.
-
K. Banik and G. Mennig. Influence of the injection molding process on the creep behavior of semicrystalline pbt during aging below its glass transition temperature. Mechanics of Time-Dependent Materials, 9(4):45–55, 2005. ISSN 1573-2738. doi: 10.1007/s11043-005-9003-9. URL https://doi.org/10.1007/s11043-005-9003-9.
-
A. Bolshakov and G. M. Pharr. Influences of pileup on the measurement of mechanical properties by load and depth sensing indentation techniques. Journal of Materials Research, 13(4):1049–1058, 1998. ISSN 2044-5326. doi: 10.1557/JMR.1998.0146. URL https://doi.org/10.1557/JMR.1998.0146.
-
B. J. Briscoe, L. Fiori, and E. Pellillo. Nano-indentation of polymeric surfaces. Journal of Physics D: Applied Physics, 31:2395–2405, 1998. ISSN 0022-3727. PII: S0022-3727(98)91154-8.
-
Yang-Tse Cheng and Che-Min Cheng. Scaling, dimensional analysis, and indentation measurements. Materials Science and Engineering: R: Reports, 44(4):91–149, 2004. ISSN 0927-796X. doi: https://doi.org/10.1016/j.mser.2004.05.001. URL https://www.sciencedirect.com/science/article/pii/S0927796X04000415.
-
G. Constantinides, K.S. Ravi Chandran, F.-J. Ulm, and K.J. Van Vliet. Grid indentation analysis of composite microstructure and mechanics: Principles and validation. Materials Science and Engineering: A, 430(1):189–202, 2006. ISSN 0921-5093. doi: https://doi.org/10.1016/j.msea.2006.05.125. URL https://www.sciencedirect.com/science/article/pii/S0921509306009294.
-
T. D. Downing, R. Kumar, W. M. Cross, L. Kjerengtroen, and J. J. Kellar. Determining the interphase thickness and properties in polymer matrix composites using phase imaging atomic force microscopy and nanoindentation. Journal of Adhesion Science and Technology, 14(14):1801–1812, 2000. doi: 10.1163/156856100743248. URL https://doi.org/10.1163/156856100743248.
-
S. El-Safty, N. Silikas, R. Akhtar, and D. C. Watts. Nanoindentation creep versus bulk compressive creep of dental resin-composites. Dental Materials, 28(11):1171–1182, 2012. ISSN 0109-5641. doi: 10.1016/j.dental.2012.08.012. URL https://www.sciencedirect.com/science/article/pii/S0109564112003995.
-
P. Eyerer, T. Hirth, and P. Elsner. Polymer Engineering: Technologien und Praxis. Springer Berlin / Heidelberg, Berlin, Heidelberg, 1 edition, 2008. ISBN 9783540724025.
-
L. Fahrmeir, C. Heumann, R. Künstler, I. Pigeot, and G. Tutz. Statistik. Springer Spektrum, Berlin, Heidelberg, 9 edition, 2024. ISBN 978-3-662-67525-0. doi: 10.1007/978-3-662-67526-7. eBook ISBN: 978-3-662-67526-7.
-
G. Feng and A. H. W. Ngan. Effects of creep and thermal drift on modulus measurement using depth-sensing indentation. Journal of Materials Research, 17(3):660–668, 2002. ISSN 2044-5326. doi: 10.1557/JMR.2002.0094. URL https://doi.org/10.1557/JMR.2002.0094.
-
Y. Gaillard and F. Amiot. Grid nano-indentation as full-field measurements. Composites Part A: Applied Science and Manufacturing, 132:105807, 2020. ISSN 1359-835X. doi: https://doi.org/10.1016/j.compositesa.2020.105807. URL https://www.sciencedirect.com/science/article/pii/S1359835X20300452.
-
R. F. Gibson. A review of recent research on nanoindentation of polymer composites and their constituents. Composites Science and Technology, 105:51–65, 2014. ISSN 0266-3538. doi: https://doi.org/10.1016/j.compscitech.2014.09.016. URL https://www.sciencedirect.com/science/article/pii/S0266353814003492.
-
J. Grondin, O. Smerdova, S. Castagnet, and C. Tomas. Intraspherulitic mechanical heterogeneities and microstructure of i-pp highlighted by nanoindentation and atomic force microscopy. Polymer, 285:126391, 2023. ISSN 0032-3861. doi: https://doi.org/10.1016/j.polymer.2023.126391. URL https://www.sciencedirect.com/science/article/pii/S0032386123007218.
-
T. S. Gross, N. Timoshchuk, I. I. Tsukrov, R. Piat, and B. Reznik. On the ability of nanoindentation to measure anisotropic elastic constants of pyrolytic carbon. ZAMM - Journal of Applied Mathematics and Mechanics, 93(5):301–312, 2013. doi: 10.1002/zamm.201100128.
-
M. Hardiman, T.J. Vaughan, and C.T. McCarthy. The effect of fibre constraint in the nanoindentation of fibrous composite microstructures: A finite element investigation. Computational Materials Science, 64:162–167, 2012. ISSN 0927-0256. doi: https://doi.org/10.1016/j.commatsci.2012.04.033. URL https://www.sciencedirect.com/science/article/pii/S0927025612002479. Proceedings of the 21st International Workshop on Computational Mechanics of Materials (IWCMM 21).
-
M. Hardiman, T. Vaughan, and C. McCarthy. The effects of pile-up, viscoelasticity and hydrostatic stress on polymer matrix nanoindentation. Polymer Testing, 52, 04 2016. doi: 10.1016/j.polymertesting.2016.04.003.
-
M. Hardiman, T.J. Vaughan, and C.T. McCarthy. A review of key developments and pertinent issues in nanoindentation testing of fibre reinforced plastic microstructures. Composite Structures, 180:782–798, 2017. ISSN 0263-8223. doi: https://doi.org/10.1016/j.compstruct.2017.08.004. URL https://www.sciencedirect.com/science/article/pii/S0263822317300211.
-
J. C. Hay, A. Bolshakov, and G. M. Pharr. A critical examination of the fundamental relations used in the analysis of nanoindentation data. Journal of Materials Research, 14(6):2296–2305, 1999. ISSN 2044-5326. doi: 10.1557/JMR.1999.0306. URL https://doi.org/10.1557/JMR.1999.0306.
-
E. D. Hintsala, U. Hangen, and D. D. Stauffer. High-throughput nanoindentation for statistical and spatial property determination. JOM, 70(4):494–503, 2018. ISSN 1543-1851. doi: 10.1007/s11837-018-2752-0. URL https://doi.org/10.1007/s11837-018-2752-0.
-
G. Hochstetter, A. Jimenez, and J. L. Loubet. Strain-rate effects on hardness of glassy polymers in the nanoscale range. comparison between quasi-static and continuous stiffness measurements. Journal of Macromolecular Science, Part B, 38(5-6): 681–692, 1999. doi: 10.1080/00222349908248131. URL https://doi.org/10.1080/00222349908248131.
20 of 22
-
Z. Hu, M. Farahikia, and F. Delfanian. Fiber bias effect on characterization of carbon fiber-reinforced polymer composites by nanoindentation testing and modeling. Journal of Composite Materials, 49(27):3359–3372, 2015. doi: 10.1177/0021998314562221.
-
C.-T. Huang, X.-W. Chen, and W.-W. Fu. Investigation on the fiber orientation distributions and their influence on the mechanical property of the co-injection molding products. Polymers, 12(1):24, 2020. ISSN 2073-4360. doi: 10.3390/polym12010024. URL https://www.mdpi.com/2073-4360/12/1/24.
-
C. Huet. Application of variational concepts to size effects in elastic heterogeneous bodies. Journal of the Mechanics and Physics of Solids, 38(6):813–841, 1990. doi: 10.1016/0022-5096(90)90041-2. URL https://www.sciencedirect.com/science/article/pii/0022509690900412.
-
M. Huszar, G. Oreski, and F. Arbeiter. Modulus estimation of polymers via nanoindentation – impact of surface roughness, peak force and testing speed. Acta Polytechnica CTU Proceedings, 50:1–6, 2024. doi: 10.14311/APP.2024.50.0001.
-
J. E. Jakes. Improved methods for nanoindentation berkovich probe calibrations using fused silica. Journal of Materials Science, 53(7):4814–4827, 2018. ISSN 1573-4803. doi: 10.1007/s10853-017-1922-8. URL https://doi.org/10.1007/s10853-017-1922-8.
-
J. E. Jakes and D. S. Stone. Best practices for quasistatic berkovich nanoindentation of wood cell walls. Forests, 12(12), 2021. ISSN 1999-4907. doi: 10.3390/f12121696. URL https://www.mdpi.com/1999-4907/12/12/1696.
-
J. E. Jakes, C. Frihart, J. F. Beecher, R. Moon, P. Resto Irizarry, Z. Melgarejo, O. Suárez, H. Baumgart, A. A. Elmustafa, and D. S. Stone. Nanoindentation near the edge. Journal of Materials Research, 24:1016–1031, 2011. doi: 10.1557/jmr.2009.0076.
-
J. E. Jakes, J. O'dell, and D. S. Stone. Viscoelastic moduli and path-dependent hardness across four decades of timescale in semicrystalline polymers from berkovich nanoindentation. JOM, 76(6):2956–2969, 2024. ISSN 1543-1851. doi: 10.1007/s11837-024-06551-0. URL http://dx.doi.org/10.1007/s11837-024-06551-0.
-
C. Jiang, M. Davis, and J. Zekonyte. Finding minimal optimal indent separation for polystyrene via instrumental nanoindentation and fea method. Applied Sciences, 10(12), 2020. ISSN 2076-3417. doi: 10.3390/app10124262. URL https://www.mdpi.com/2076-3417/10/12/4262.
-
M. Kaliske. A formulation of elasticity and viscoelasticity for fibre reinforced material at small and finite strains. Computer Methods in Applied Mechanics and Engineering, 185(2): 225–243, 2000. ISSN 0045-7825. doi: https://doi.org/10.1016/S0045-7825(99)00261-3. URL https://www.sciencedirect.com/science/article/pii/S0045782599002613.
-
S. K. Khanna, P. Ranganathan, S. B. Yedla, R. M. Winter, and K. Paruchuri. Investigation of nanomechanical properties of the interphase in a glass fiber reinforced polyester composite using nanoindentation. Journal of Engineering Materials and Technology, 125(2):90–96, 2003. ISSN 0094-4289. doi: 10.1115/1.1543966. URL https://doi.org/10.1115/1.1543966.
-
E. Klatt and N. Rauter. Stochastic modelling of the spatially distributed viscoelasticity of short fiber-reinforced composites using random fields. In Proceedings of the 24th International Conference on Composite Materials (ICCM24), Baltimore, MD, USA, 2025.
-
E. Klatt, B. Zimmering, O. Niggemann, and N. Rauter. Machine-learning-enabled comparative modelling of the creep behaviour of unreinforced pbt and short-fibre reinforced pbt using prony and fractional derivative models. Applied Mechanics, 6(3), 2025. ISSN 2673-3161. doi: 10.3390/applmech6030060. URL https://www.mdpi.com/2673-3161/6/3/60.
-
R. Kumar, W.M. Cross, L. Kjerengtroen, and J.J. Kellar. Fiber bias in nanoindentation of polymer matrix composites. Composite Interfaces, 11(5-6):431–440, 2004. doi: 10.1163/1568554042246215. URL https://doi.org/10.1163/1568554042246215.
-
S.-H. Lee, S. Wang, G. M. Pharr, and H. Xu. Evaluation of interphase properties in a cellulose fiber-reinforced polypropylene composite by nanoindentation and finite element analysis. Composites Part A: Applied Science and Manufacturing, 38(6): 1517–1524, 2007. ISSN 1359-835X. doi: https://doi.org/10.1016/j.compositesa.2007.01.007. URL https://www.sciencedirect.com/science/article/pii/S1359835X07000139.
-
Q. P. McAllister, J. W. Gillespie, and M. R. VanLandingham. Evaluation of the three-dimensional properties of kevlar across length scales. Journal of Materials Research, 27(14):1824–1837, 2012. ISSN 0884-2914. doi: 10.1557/jmr.2012.80. URL https://www.cambridge.org/core/article/evaluation-of-the-threedimensional-properties-of-kevlar-across-length-scaleE261AE36D6E4064FDA682B36877C528A.
-
Y. Meng, S. Wang, Z. Cai, T. M. Young, G. Du, and Y. Li. A novel sample preparation method to avoid influence of embedding medium during nano-indentation. Applied Physics A, 110(2): 361–369, 2013. ISSN 1432-0630. doi: 10.1007/s00339-012-7123-z. URL https://doi.org/10.1007/s00339-012-7123-z.
-
N. Moharrami and S.J. Bull. A comparison of nanoindentation pile-up in bulk materials and thin films. Thin Solid Films, 572: 189–199, 2014. ISSN 0040-6090. doi: https://doi.org/10.1016/j.tsf.2014.06.060. URL https://www.sciencedirect.com/science/article/pii/S00406090014008189. The 41st International Conference on Metallurgical Coatings and Thin Films.
-
A. H. W. Ngan and B. Tang. Viscoelastic effects during unloading in depth-sensing indentation. Journal of Materials Research, 17 (10):2604–2610, 2002. ISSN 2044-5326. doi: 10.1557/JMR.2002.0377. URL https://doi.org/10.1557/JMR.2002.0377.
-
W. D. Nix and H. Gao. Indentation size effects in crystalline materials: A law for strain gradient plasticity. Journal of the Mechanics and Physics of Solids, 46(3):411–425, 1998. ISSN 0022-5096. doi: https://doi.org/10.1016/S0022-5096(97)00086-0. URL https://www.sciencedirect.com/science/article/pii/S0022509697000860.
-
W C Oliver and G M Pharr. An improved technique for determining hardness and elastic modulus using load and displacement sensing indentation experiments. Journal of Materials Research; (United States), 7(6):1564–1583, 1992. ISSN 0884-2914. doi: 10.1557/JMR.1992.1564. URL https://www.osti.gov/biblio/7238008.
-
W. C. Oliver and G. M. Pharr. Measurement of hardness and elastic modulus by instrumented indentation: Advances in understanding and refinements to methodology. Journal of Materials Research, 19(1):3–20, 2004. ISSN 0884-2914. doi: 10.1557/jmr.2004.19.1.3. URL https://www.cambridge.org/core/article/measurement-of-hardness-and-elastic-modulus-by-instrumented-indentationD81F6EBA71598A8C6EE338BF5A3D5AE7.
-
M. Ostoja-Starzewski. Material spatial randomness: From statistical to representative volume element. Probabilistic Engineering Mechanics, 21(2):112–132, 2006. ISSN 0266-8920. doi: https://doi.org/10.1016/j.probengmech.2005.07.007. URL https://www.sciencedirect.com/science/article/pii/S0266892005000433.
-
M. Ovsik, V. Senkerik, D. Manas, and M. Stanek. The behaviour of cross-linking filled PBT measured by nano-hardness. MM Science Journal, page 1110, Oct. 2016. doi: 10.17973/MMSJ.2016_10_201678.
-
P. S. Phani and W.C. Oliver. A critical assessment of the effect of indentation spacing on the measurement of hardness and modulus using instrumented indentation testing. Materials & Design, 164:107563, 2019. ISSN 0264-1275. doi: https://doi.org/10.1016/j.matdes.2018.107563.
-
G. M. Pharr and A. Bolshakov. Understanding nanoindentation unloading curves. Journal of Materials Research, 17(10):2660–2671, 2002. ISSN 2044-5326. doi: 10.1557/JMR.2002.0386. URL
21 of 22 https://doi.org/10.1557/JMR.2002.0386.
-
N. Rauter. A computational modeling approach based on random fields for short fiber-reinforced composites with experimental verification by nanoindentation and tensile tests. Computational Mechanics, 67(2):699–722, 2021. ISSN 1432-0924. doi: 10.1007/s00466-020-01958-3. URL https://doi.org/10.1007/s00466-020-01958-2.
-
N. Rauter. Probabilistic modeling of short fiber-reinforced composites taking into account finite deformations – numerical modeling and experimental validation –, 2023. URL https://openhsu.ub.hsu-hh.de/handle/10.24405/14977.
-
N. Rauter and R. Lammering. Experimental characterization of short fiber-reinforced composites on the mesoscale by indentation tests. Applied Composite Materials, 28(5):1747–1765, 2021. ISSN 1573-4897. doi: 10.1007/s10443-021-09937-4. URL https://doi.org/10.1007/s10443-021-09937-4.
-
E. Rossi, J. M. Wheeler, and M. Sebastianian. High-speed nanoindentation mapping: A review of recent advances and applications. Current Opinion in Solid State and Materials Science, 27(5):101107, 2023. ISSN 1359-0286. doi: https://doi.org/10.1016/j.cossms.2023.101107. URL https://www.sciencedirect.com/science/article/pii/S1359028623000529.
-
P. Sarkar and S. Verma. Phenomena-based optimization of load function during nanoindentation experiments for estimating elastic aspect of viscous materials. Polymer, 302:127059, 2024. ISSN 0032-3861. doi: https://doi.org/10.1016/j.polymer.2024.127059. URL https://www.sciencedirect.com/science/article/pii/S003238612400394X.
-
P. Sarkar and S. Verma. Investigation of creep effect on cyclic nanoindentation deformation properties in thermoplastic glassy polymers. Journal of Polymer Research, 33(2), 2026. ISSN 1572-8935. doi: 10.1007/s10965-026-04788-8. URL https://doi.org/10.1007/s10965-026-04788-8.
-
P. Sarkar, P. Pant, and H. Nanavati. Physical phenomena during nanoindentation deformation of amorphous glassy polymers. Polymer, 312:127597, 2024. ISSN 0032-3861. doi: https://doi.org/10.1016/j.polymer.2024.127597. URL https://www.sciencedirect.com/science/article/pii/S0032386124009339.
-
S. Shen, H. Li, L. Yang, N. Li, J. Wu, and T. Zhao. High-throughput screening the micro-mechanical properties of polyimide matrix composites at elevated temperatures. Polymer Testing, 107:107483, 2022. ISSN 0142-9418. doi: https://doi.org/10.1016/j.polymertesting.2022.107483. URL https://www.sciencedirect.com/science/article/pii/S0142941822000125.
-
K. Shirasu, K. Goto, and K. Naito. Microstructure-elastic property relationships in carbon fibers: A nanoindentation study. Composites Part B: Engineering, 200:108342, 2020. ISSN 1359-8368. doi: https://doi.org/10.1016/j.compositesb.2020.108342. URL https://www.sciencedirect.com/science/article/pii/S1359836820333916.
-
A. Slagter, J. Everaerts, and A. Mortensen. Nanoindentation of embedded particles. Journal of Materials Research, 38(6):1694–1705, 2023. ISSN 2044-5326. doi: 10.1557/s43578-023-00920-2. URL https://doi.org/10.1557/s43578-023-00920-2.
-
M. Slouf, M. Steinhart, P. Nemecek, V. Gajdosova, and J. Hordan. Correlations between microscale indentation creep and macroscale tensile creep of polymers. Materials, 16(2), 2023. ISSN 1996-1944. doi: 10.3390/ma16020834. URL https://www.mdpi.com/1996-1944/16/2/834.
-
I. N. Sneddon. The relation between load and penetration in the axisymmetric boussinesq problem for a punch of arbitrary profile. International Journal of Engineering Science, 3(1):47–57, 1965. ISSN 0020-7225. doi: https://doi.org/10.1016/0020-7225(65)90019-4. URL https://www.sciencedirect.com/science/article/pii/0020722565900194.
-
D. Tranchida, S. Piccarolo, J. Loos, and A. Alexeev. Mechanical characterization of polymers on a nanometer scale through nanoindentation. a study on pile-up and viscoelasticity. Macromolecules, 40(4):1259–1267, 2007. doi: 10.1021/ma062140k.
-
M. Troyon and S. Lafaye. About the importance of introducing a correction factor in the sneddon relationship for nanoindentation measurements. Philosophical Magazine, 86(33-35):5299–5307, 2006. doi: 10.1080/14786430600606834. URL https://doi.org/10.1080/14786430600606834.
-
F.-J. Ulm, M. Vandamme, H. M. Jennings, J. Vanzo, M. Bentivegna, K. J. Krakowiak, G. Constantinides, C. P. Bobko, and K. J. Van Vliet. Does microstructure matter for statistical nanoindentation techniques. Cement and Concrete Composites, 32(1): 92–99, 2010. ISSN 0958-9465. doi: https://doi.org/10.1016/j.cemconcomp.2009.08.007. URL https://www.sciencedirect.com/science/article/pii/S0958946509001425.
-
M. R. VanLandingham, N.-K. Chang, P. L. Drzal, C. C. White, and S.-H. Chang. Viscoelastic characterization of polymers using instrumented indentation. i. quasi-static testing. Journal of Polymer Science Part B: Polymer Physics, 43(14):1794–1811, 2005. doi: https://doi.org/10.1002/polb.20454. URL https://onlinelibrary.wiley.com/doi/abs/10.1002/polb.20454.
-
W. Yan, C. L. Pun, Z. Wu, and G. P. Simon. Some issues on nanoindentation method to measure the elastic modulus of particles in composites. Composites Part B: Engineering, 42(8): 2093–2097, 2011. ISSN 1359-8368. doi: https://doi.org/10.1016/j.compositesb.2011.05.002. URL https://www.sciencedirect.com/science/article/pii/S135983681100196X. Special Issue on Preparation, Properties and Applications of Nanocomposites.
-
T. I. Zohdi and P. Wriggers. An Introduction to Computational Micromechanics, volume 20 of Lecture Notes in Applied and Computational Mechanics. Springer, Berlin, Heidelberg, corrected second printing edition, 2008. ISBN 978-3-540-77482-2. doi: 10.1007/978-3-540-32360-0. URL https://link.springer.com/book/10.1007/978-3-540-32360-0.
-
Product Information ZHN – Universal Nanomechanical Testing System. ZwickRoell GmbH & Co. KG, 2026. URL https://www.zwickroell.com/fileadmin/content/Files/SharePoint/user_upload/PI_EN/15_901_ZHN_PI_EN.pdf. PDF-Document.
22 of 22